Frontier Insights: Geometric Determinants of Sinterless, Low-Temperature-Processed 3D Nanoprinted Glass

玉之泉

Introduction: Conventional top-down glass microfabrication methods (such as etching and lithography) face geometric constraints when constructing complex three-dimensional structures, making it difficult to meet the demands of micro/nano systems for complex 3D architectures. Existing 3D glass printing technologies either require high-temperature sintering (e.g. 1300°C), which limits equipment accessibility, or suffer from nanoparticle suspensions that limit feature resolution. Studies have shown that polyhedral oligomeric silsesquioxane (POSS) resins can be converted into fused silica glass by low-temperature (650°C) thermal decomposition without sintering, but for larger microstructures printed with this technology (e.g. ≥25μm thick), little is known about how their optical and mechanical properties change, which limits the use of the technology in micro/nano systems that integrate features of different thicknesses (such as micro-optics, microneedles and microfluidics). In other thermal-decomposition-based two-photon direct laser writing (DLW) 3D printing systems, heat treatment imposes a limit on the maximum resolvable feature size, but whether similar constraints exist for POSS-based DLW printing remains unclear, making it impossible to determine the applicable range of this technology for glass microstructures with features of different thicknesses. To address these issues, a research team at the University of Maryland published a paper titled "Geometric determinants of sinterless, low-temperature-processed 3D-nanoprinted glass" in the journal Microsystem & Nanoengineering, investigating the effect of feature size on the optical and mechanical properties of 3D-printed fused silica glass microstructures that are sinterless and low-temperature (650°C) post-processed, providing key benchmarks for glass microstructure design in micro/nano system applications.

Abstract: Glass materials are essential in microsystem applications ranging from optics and photonics to microfluidics and biomedicine, driving growing interest in additive manufacturing (i.e. 3D printing) for glass micro/nanotechnology. Notably, recent studies have shown that three-dimensional nanostructured fused silica glass components can be fabricated by two-photon direct laser writing (DLW) of organic-inorganic hybrid polyhedral oligomeric silsesquioxane (POSS)-based resins, a discovery of unique promise, especially because it offers the advantage of sinterless, low-temperature (i.e. 650°C) post-processing. However, it is not yet known how 3D printing larger glass microstructures (e.g. with feature thickness ≥25μm) by such methods affects key material properties such as the final optical and mechanical characteristics. To fill this knowledge gap, this study investigates DLW-printed feature size as a key determinant of the optical and mechanical properties of POSS-based fused silica glass microstructures. Experiments on TPP-DLW-printed microlenses showed comparable optical transparency at initial thicknesses up to 40μm, but transmittance dropped significantly from 87.87±1.18% to 63.57±5.10% when the thickness increased to 60μm. Similarly, compressive loading studies of hollow glass cylindrical microstructures showed stable performance at initial DLW-printed wall thicknesses up to 30μm, but a significant decline beyond that thickness, for example from 251.6±71.9MPa at 30μm to 99.7±63.9MPa at 40μm in Young's modulus. As an exemplary case relevant to biomedical microinjection applications, we used this new knowledge to fabricate POSS-based glass microneedle arrays (MNAs) by DLW printing and demonstrated that they can penetrate media that standard polymer microneedle arrays cannot. Overall, this study establishes the key optical and mechanical benchmarks that underpin the utility of DLW 3D-printed POSS-based fused silica glass microstructures in emerging applications.


Article highlights:


Technological breakthrough: For the first time, container-based DLW was used to print POSS resin (the POSS-based resin and other photomaterials are loaded into a container, and a femtosecond infrared laser scans point by point and layer by layer through the photomaterial in the container, selectively photopolymerizing the resin via two-photon polymerization to achieve 3D printing of micro/nanostructures), overcoming the height limitations of conventional oil-immersion and dip-in laser lithography (DiLL) and enabling glass microstructures up to 1mm, an order of magnitude improvement over previous reports.

Process optimization: For the first time, adaptive resolution printing in dynamic optical tuning (DOT) was applied to POSS-based materials, reducing surface defects, improving optical quality and shortening printing time by dynamically adjusting the voxel size.

Performance benchmarks: The critical feature sizes of POSS-based DLW-printed glass were identified (60μm critical thickness for optical performance and 40μm critical wall thickness for mechanical performance), providing a quantitative basis for microstructure design.

Application validation: The advantages of glass microneedle arrays in biomedicine were demonstrated: they can penetrate 10% agarose gel (simulating cartilage/tendon tissue), which polymer microneedles cannot.

玉之泉

Figure 1 Schematic of the feature size determinants of POSS-based TPP-DLW 3D-printed fused silica glass

a: Molecular composition of the POSS resin, including acrylate-functionalized POSS monomers, trifunctional acrylate monomers and a photoinitiator.

b-c: DLW printing process: the resin is loaded into a container, and a femtosecond infrared laser scans point by point and layer by layer to induce two-photon polymerization, forming a crosslinked polymer structure containing POSS cage-like nanoclusters.

d-e: Conversion into glass by low-temperature thermal decomposition (650°C): when the feature thickness (t) exceeds the critical thickness (tcr), cracks appear and optical and mechanical performance decline; when t < tcr, the structure converts into pure fused silica glass.

玉之泉

Figure 2 Fabrication results

a-c: Micrographs of the DLW printing process for different structures:

a: Microlens (total printing time ≈16 minutes); b: hollow cylinder (≈20 minutes); c: microneedle array (≈44 minutes); scale bars are 500μm.

d: Thermal post-processing protocol: room temperature →450°C (0.5°C/min, hold 24 hours) →650°C (0.5°C/min, hold 1 hour) →room temperature (-1.5°C/min).

e: Thermogravimetric analysis (TGA): the final residual mass is 36.57% of the initial mass, with minimal mass change after 600°C, indicating that thermal decomposition is nearly complete.

f: Energy dispersive spectroscopy (EDS): characteristic peaks of Si and O were detected with an atomic ratio of ≈1:2, consistent with SiO₂ and verifying successful glass conversion.

玉之泉

Figure 3 Fabrication and optical characterization of POSS-based DLW-printed fused silica glass microlenses

a-b: Schematic of the microlens structure:

The lens is embedded in a lattice support (to assist handling); a is an overall view and b a cross-sectional view.

c-l: Images of microlenses with different initial thicknesses:

c,h: 20μm thick (no defects); d,i: 40μm thick (no defects); e,j: 60μm thick (cracks); f,k: 80μm thick (cracks); g,l: 100μm thick (cracks). Observed under bright-field microscopy (c-g) and SEM (h-l); scale bars 50μm (25μm for magnified views).

m: Transmittance data: no significant difference between 20μm (86.75±2.42%) and 40μm (87.87±1.18%); significant decreases at 60μm (63.57±5.10%), 80μm (58.79±9.92%) and 100μm (52.20±8.29%) (p<0.005).

玉之泉

Figure 4 Compression test results for polymer hollow cylinders before heat treatment

a: Micrographs of the compression process, showing the cylinder from its initial state through deformation to failure.

b: Young's modulus data: no significant difference for polymer structures with 6-30μm wall thickness (all are intrinsic polymer properties).

c: Failure force data: as the wall thickness increases (6-30μm), the failure force gradually increases, consistent with structural mechanics expectations.

玉之泉

Figure 5 Numerical simulation and compression test results of fused silica glass hollow cylinders

a-c: Numerical simulation:

a: Schematic of compression deformation; b: stress-strain curves for different wall thicknesses (linear elastic); c: reaction force at 25μm deformation increases with wall thickness.

d-h: SEM images of glass cylinders after thermal decomposition: final wall thicknesses of about 6μm (d), 12μm (e), 18μm (f), 24μm (g) and 30μm (h); cracks appear above 40μm.

i: Micrographs of the compression process of a glass cylinder.

j-k: Experimental data:

j: Young's modulus: significant decreases at 30μm (251.6±71.9MPa), 40μm (99.7±63.9MPa) and 50μm (42.9±27.4MPa) (p<0.005);

k: Failure force: significant decreases at 30μm (5.09±2.12N), 40μm (2.46±3.97N) and 50μm (0.71±0.61N) (p<0.05/p<0.01).

玉之泉

Figure 6 Penetration experiments of microneedle arrays (MNA) in 10% agarose gel

a: Polymer control group: the microneedles broke during the penetration attempt and could not penetrate.

b: Glass MNA group: penetrated and removed successfully, leaving visible penetration marks; scale bar 500μm.

c: Quantification of penetration depth: the actual penetration depth of the glass MNA (653±32μm) matched the expected value (697μm), while the polymer group showed no penetration.

This study focuses on two-photon direct laser writing (DLW) 3D nanoprinting based on polyhedral oligomeric silsesquioxane (POSS) resin, examining how feature size affects the optical and mechanical properties of 3D-printed fused silica glass microstructures that are sinterless and post-processed at a low temperature of 650°C. Glass materials are widely used in many microsystem fields, and the method of DLW printing POSS-based resin followed by low-temperature thermal decomposition into fused silica glass is promising, but the performance of larger microstructures was previously unclear. For optical properties, the study found that microlenses with initial thicknesses ≤40μm maintained a stable transmittance of about 87%, while at initial thicknesses ≥60μm it dropped significantly to below 63.57%; for mechanical properties, hollow cylinders with initial wall thicknesses ≤30μm showed stable compression performance (Young's modulus about 251.6MPa), while performance dropped sharply at initial wall thicknesses ≥40μm (Young's modulus down to 99.7MPa). On this basis, the glass microneedle arrays prepared by the team were able to penetrate biological substitute materials that polymer microneedles could not, validating the application value of the technology in biomedicine and other fields and establishing key optical and mechanical benchmarks for glass microstructure design in related micro/nano system applications.



Source: Colton, A., Halli, R.N., Ma, M.R. et al. Geometric determinants of sinterless, low-temperature-processed 3D-nanoprinted glass. Microsyst Nanoeng 11, 145 (2025). https://doi.org/10.1038/s41378-025-00983-7

Article URL: https://www.nature.com/articles/s41378-025-00983-7