Introduction: Bioactive glass (BG) is highly attractive in tissue engineering because it bonds rapidly with bone and promotes new bone formation. Its pore structure is critical for cell infiltration, nutrient supply, and bone ingrowth, but conventional additive manufacturing (AM) struggles to realize features below 100μm. Researchers at the Department of Microsystems Engineering, University of Freiburg, were the first to use two-photon lithography (TPL) to construct BG microscaffolds with single-micron features, in order to investigate how scaffold microstructure affects cell behavior. By combining TPL with heat treatment, they successfully produced BG microscaffolds with high resolution (minimum feature size down to 6μm). In vitro experiments showed that the scaffolds are bioactive in simulated body fluid (SBF), inducing hydroxycarbonate apatite (HCA) formation, and are cytocompatible with human mesenchymal stromal cells (MSCs), offering new possibilities for bone tissue engineering and cell culture. The related paper, “Bioactive Glass Microscaffolds Fabricated by Two-Photon Lithography,” was published in ADVANCED MATERIALS.
Abstract: Porous scaffolds made of bioactive glass (BG) have attracted much attention in tissue engineering because they bond rapidly to bone and promote new bone formation. Pores and channels of 100 to 500 micrometers provide space for cell infiltration and nutrient supply, supporting bone ingrowth and vascularization. In addition, smaller pores and structural features of a few micrometers influence cell behavior such as adhesion and osteogenic differentiation. Additive manufacturing (AM) is well suited to producing such geometries. However, microstructuring bioactive glass is demanding, and conventional additive manufacturing cannot achieve features below 100 micrometers. In this work, bioactive glass was structured with single-micron features by two-photon lithography (TPL) for the first time. A composite containing bioactive glass nanoparticles was structured by TPL, and glass scaffolds were obtained by heat treatment. The glass used in this study showed in vitro bioactivity in simulated body fluid (SBF) and cytocompatibility with human mesenchymal stromal cells (MSCs), making it a suitable material for tissue engineering. This process provides a toolbox for shaping a variety of existing bioactive glass particles with features as small as 6 micrometers, and will broaden understanding of how scaffold design influences cell behavior.
Microstructure fabrication and properties: A variety of complex 3D scaffolds were successfully produced, such as 2.5D pillar arrays (beam width 6μm), buckyballs (pores as small as 30μm), gyroid lattices (wall thickness 15μm), and a model of human cancellous bone (dimensions up to 10mm×7.0mm×1.5mm, struts as small as 63μm). After heat treatment at 900°C, the scaffolds showed a linear shrinkage of 9%, a porosity of 49.7%, and a Vickers hardness of 147HV, higher than that of human bone (33-42HV).
Bioactivity and cytocompatibility: After immersion in SBF for 3 weeks, an HCA layer formed on the scaffold surface, with a Ca/P ratio of 1.6 (close to stoichiometric hydroxyapatite); the viability of human MSCs on the scaffolds was comparable to that on tissue culture plastic, and ALP activity indicated support for differentiation toward osteoblasts, with cells showing a spindle-like morphology on the scaffold surface, demonstrating good cell-material interactions.

Figure 1 Microstructuring of BG using TPL
a) SEM image of BG nanoparticles prepared by a modified Stöber synthesis; scale bar 500nm.
b) Schematic of microstructuring BG by TPL inside a vat.
c) After printing, the parts are heat-treated at 900°C to obtain pure BG structures; during processing the organic binder decomposes and the parts shrink; scale bar 1mm.
d) TGA shows that binder decomposition is complete at 500°C; shrinkage during heat treatment was characterized by dilatometry.
e) During heat treatment from 700°C to 1200°C, Vickers hardness increases and surface area decreases, indicating consolidation of the nanoparticles.
f) XRD analysis shows that crystallization occurs above 900°C.

Figure 2 BG lattices fabricated by TPL and heat-treated at 900°C
a) 2.5D structures, such as a pillar array with beam widths of 6μm and a height of 10μm; scale bar 30μm.
b) Buckyballs with pores as small as 30μm; scale bar 100μm.
c) Gyroid lattice; scale bar 150μm.
d) Truncated octahedron lattice; scale bar 200μm.
e) Fabricated human cancellous bone model with a length of 1cm; scale bar 4mm.
f) Structure containing high-resolution features; scale bar 200μm.

Figure 3 Biological characterization of BG after heat treatment at 900°C
a-d) In vitro mineralization of BG studied by SEM after immersion in SBF for 3 days, 1 week, 2 weeks, and 3 weeks, showing the growth of HCA on the BG surface; all scale bars 500nm.
e) Cytocompatibility of BG examined by a cell viability assay with tissue culture plastic as the reference; the data show that cell viability on BG is similar to that on tissue culture plastic.
f) Osteogenic differentiation of MSCs toward osteoblasts characterized by ALP assay; BG permits differentiation, comparable to fused silica and tissue culture plastic.
g) Cell morphology visualized by staining of cancellous bone scaffolds made of BG; scale bar 60μm.
This study achieved high-resolution microstructuring of BG by TPL for the first time. The resulting scaffolds combine nanoscale features with macroscopic dimensions (up to 1cm), providing a new material platform for bone tissue engineering. The method expands the application of BG in complex three-dimensional structures and is expected to reveal in depth how microscopic scaffold design regulates cell behavior, advancing the development of personalized bone repair materials.
Source: Hambitzer,Leonhard et al."Bioactive Glass Microscaffolds Fabricated by Two-Photon Lithography",Adv.Mater.2025,2504475.
Article URL:https://advanced.onlinelibrary.wiley.com/doi/10.1002/adma.202504475