Insights: Resonant Scanner Boosts Two-Photon Polymerization Throughput

Yuzhiquan

Introduction: A 3D printing and biofabrication research group at the Institute of Materials Science and Technology, TU Wien, recently proposed a two-photon polymerization (TPP) system based on a resonant scanner, aiming to solve the low throughput of 2PP and improve the efficiency of tissue engineering microscaffold fabrication. The results were published in January 2025 in the journal Additive Manufacturing under the title “Two-photon polymerization system based on a resonant scanner for high-throughput production of tissue engineering microscaffolds.”

Abstract: Two-photon polymerization (TPP) is a 3D printing technique known for its outstanding resolution and its ability to produce complex structures directly within a volume of material. Although the technique has largely matured since its first demonstration, the long processing times caused by high resolution remain a major obstacle to using TPP in production. This study introduces a novel TPP setup designed to address this limitation by significantly increasing throughput—by at least an order of magnitude compared with existing commercial products. This improvement is achieved by implementing resonant scanning technology, which rapidly guides the laser during fabrication. All optical components were carefully selected to avoid any limitations that could arise once the scanner is no longer the sole bottleneck for production throughput. In addition, newly developed characterization and calibration methods for optimizing structuring accuracy and throughput are discussed.

This study used Michler's ethyl ketone as the photoinitiator, with different resins for different tests. A 2PP system was built, comprising a femtosecond oscillator, an acousto-optic modulator (AOM), and other components, and controlled by Python code. The system was calibrated and tested through various methods, including line tests, AOM bandwidth measurements, and trigger accuracy measurements.

The AOM modulation bandwidth was determined to be about 15MHz, with a minimum feature size of 0.97µm in the scanning direction and 1.38-2.17µm at the center perpendicular to the scanning direction. Calibration work was completed, including resonant motion correction and synchronization, scaling, galvanometer motion characterization, and field-of-view (FOV) power distribution. After optimizing the microscaffold arrangement and data transmission speed, system throughput increased significantly—57 times higher than that of a conventional galvanometer scanning system.

The system greatly increases throughput and can significantly shorten production time in the fabrication of tissue engineering microscaffolds. In the future, resolution can be improved by using objectives with higher numerical aperture, but challenges remain, such as exposure time variation caused by the sinusoidal motion of the resonant scanner and the modulation bandwidth limit of the AOM.

Yuzhiquan

Figure 1: Schematic of the developed 2PP system setup. AOM: acousto-optic modulator; CM: chirped mirror; BE: beam expander consisting of two lenses; SL: scan lens; TL: tube lens; DM: dichroic mirror; OBJ: 10✖NA0.4 microscope objective.

Yuzhiquan

Figure 2 AOM bandwidth measurement and line tests

(a) Blue: measured laser amplitude when the AOM is driven with two 16ns pulses (blue), compared with a single on-switching process (orange). The pulses cannot be resolved, and the signal never reaches full amplitude. Oscillations within the signal are caused by the 80MHz repetition rate of the laser.

(b) Bandwidth test with 32ns pulses. The pulses are clearly resolved and reach full amplitude, indicating a modulation bandwidth of 30MHz.

(c) SEM image of a 20μm-long single-voxel line printed along the scanning direction, with a width of 0.97μm.

(d) Individual voxels in a continuous scan line, perpendicular to the scanning direction.

Yuzhiquan

Figure 3 Synchronization delay

(a) Comparison of different synchronization delay settings (1033-1267ns/62-76 samples) at a sampling rate of 60MSamples/s; incorrect delay settings cause frayed lines at object edges (indicated by the red arrow in one of the squares), whereas the correct delay (1167ns) produces a clean square;

(b) The delay duration increases linearly with the sampling rate. The fixed offset represents the trigger delay of the AWG.

Yuzhiquan

Figure 4 Evaluation of galvanometer scanner jump delay

(a) Cubes generated for manual evaluation of the jump delay, with incorrect settings (top) and correct settings (bottom); rows misplaced due to incorrect delay are marked with red arrows.

(b) Comparison between the galvanometer scanner control signal (orange) and the actual scanner position measured with a PSD sensor (blue). The scanner does not follow the step shape but moves with a delay. The figure shows the behavior of the galvanometer scanner during a 50μm jump. The necessary jump delay is determined as the time required for the difference between the galvanometer position and the control signal (green) to return to its pre-jump level. The magnified section shows the response delay.

(c) Measured jump delay for each jump distance.

Yuzhiquan

Figure 5 SEM images of the produced microscaffolds

(a) Power distribution of the setup across the FOV; over the entire 2650μm FOV of the objective (white circle), the power remains above 80% of the maximum.

(b) Overview of 7✖7 microscaffolds printed within one FOV. The red circle indicates the 2650μm objective FOV.

(c) Top view of the microscaffold at the center of the FOV.

(d) 45-degree view of the central microscaffold. The pillars are slightly elongated along the Z direction, as expected with the focusing optics implemented.

Yuzhiquan


Yuzhiquan



Source: Binder S, Chalupa-Gantner F, Yoo H W, et al. Two-photon polymerization system based on a resonant scanner for high-throughput production of tissue engineering microscaffolds[J]. Additive Manufacturing, 2025, 97: 104601.

Article URL:https://www.sciencedirect.com/science/article/pii/S221486042400647X?via%3Dihub

DOI:https://doi.org/10.1016/j.addma.2024.104601